1.1 ,This test method describes the inductively coupled plasma atomic emission spectrometric analysis of nickel alloys, such as specified by Committee B02, and having chemical compositions within the following limits:
Element | Application Range (%) |
Aluminum | 0.01–,1.00 |
Boron | 0.001–,0.050 |
Calcium | 0.001–,0.05 |
Carbon | 0.10–,0.20 |
Chromium | 0.01–,33.0 |
Cobalt | 0.10–,20.0 |
Copper | 0.01–,3.00 |
Iron | 0.01–,50.0 |
Lead | 0.001–,0.01 |
Magnesium | 0.0001–,0.100 |
Manganese | 0.01–,3.0 |
Molybdenum | 0.01–,30.0 |
Niobium | 0.01–,6.0 |
Nickel | 25.0–,80.0 |
Nitrogen | 0.001–,0.20 |
Oxygen | 0.0001–,0.003 |
Phosphorous | 0.001–,0.030 |
Sulfur | 0.0001–,0.010 |
Silicon | 0.01–,1.50 |
Tantalum | 0.005–,0.10 |
Tin | 0.001–,0.020 |
Titanium | 0.001–,6.0 |
Tungsten | 0.01–,5.0 |
Vanadium | 0.01–,1.0 |
Zirconium | 0.01–,0.10 |